ALLOYS USED IN BOILER
ALLOY  | 
    APPLICATIONS  | 
    TºC  | 
    ATMOSPHERE  | 
    ADVANTAGES  | 
  ||
AFNOR  | 
    AISI UNS  | 
    WERK STOFF  | 
	||||
Z6CNT 18.10  | 
    321  | 
    1.4541  | 
    Annealing - Grids  | 
    max. 750  | 
    oxidizer / inert  | 
    Basic alloys at low temperatures  | 
  
Z7CNS 20.12  | 
    302B  | 
    1.4828  | 
    Annealing - Grids  | 
    750-950  | 
    oxidizer / inert  | 
    Economic Alloy for average temperatures without phase "sigma"  | 
  
Z8CN 25.20  | 
    310 314  | 
    1.4845 1.4841  | 
    Annealing - Grids Conveyor belts  | 
    900-1100  | 
    oxidizer / inert  | 
    Good thermal characteristic, price - manufacturing good relation  | 
  
Z4CN 36.18  | 
    330  | 
    1.4864  | 
    Annealing - Grids Conveyor belts  | 
    max. 1050  | 
    cementation  | 
    Good features in cementing  | 
  
Z4CNb 36.18  | 
    330Nb  | 
    -  | 
    Grids Conveyor belts  | 
    max. 1100  | 
    cementation  | 
    Improved mechanical behaviour to 330 with addition of Nb  | 
  
NiCr 15 Fe  | 
    6600  | 
    2.4816  | 
    Annealing - Grids Conveyor belts  | 
    max. 1150  | 
    cementation  | 
    Prevents depositions in vacuum furnaces  | 
  
NiCr 23 Fe A  | 
    6601  | 
    2.4851  | 
    Annealing - Grids Conveyor belts  | 
    max. 1150  | 
    oxidizer/ presence of S  | 
    Presence of Al improves resistance against S and better mechanical properties than NiCr 15 Fe  | 
  
Request the complete technical file of the alloy.
Work other alloys on demand. 
ALLOYS USED IN FOUNDRY
COMPOSITION  | 
    HEAT TREATMENT MATERIALS  | 
  |||||||||||
HR7  | 
    HR6  | 
    HR6Nb  | 
    HR17  | 
    HR9  | 
    HR3Nb  | 
    HR5  | 
    HR32  | 
    HR23  | 
    HR4  | 
    HR1  | 
    HR27AI  | 
  |
1.4837  | 
    1.4848  | 
    HRZ  | 
    1.4806  | 
    1.4855  | 
    1.4852  | 
    1.4865  | 
    1.4849  | 
    2.4879  | 
    2.4680  | 
    Mancellium  | 
  ||
C(%)  | 
    0.43  | 
    0.46  | 
    0.3  | 
    0.5  | 
    0.15  | 
    0.43  | 
    0.4  | 
    0.45  | 
    0.45  | 
    0.6  | 
    0.06  | 
    0.1  | 
  
Mn(%)  | 
    1.4  | 
    1.0  | 
    0.9  | 
    1.0  | 
    1.0  | 
    1.0  | 
    1.0  | 
    1.0  | 
    1.0  | 
    1.2  | 
    0.1  | 
    0.55  | 
  
Si(%)  | 
    1.7  | 
    1.7  | 
    1.3  | 
    1.8  | 
    1.5  | 
    2.1  | 
    1.8  | 
    1.8  | 
    1.5  | 
    1.8  | 
    0.3  | 
    0.38  | 
  
Pmax(%)  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.035  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.015  | 
    0.03  | 
  
Smax(%)  | 
    0.025  | 
    0.025  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.025  | 
    0.03  | 
    0.03  | 
    0.03  | 
    0.015  | 
    0.03  | 
  
Cr(%)  | 
    25.0  | 
    25.0  | 
    >24  | 
    15.5  | 
    20.0  | 
    25.0  | 
    18.0  | 
    18.0  | 
    28.0  | 
    17.5  | 
    48.5  | 
    16.0  | 
  
Ni(%)  | 
    12.5  | 
    20.0  | 
    <22  | 
    35.0  | 
    34.0  | 
    34.0  | 
    37.0  | 
    37.0  | 
    48.5  | 
    51.0  | 
    BAL  | 
    75.0  | 
  
Nb(%)  | 
    -  | 
    -  | 
    Si  | 
    -  | 
    1.5  | 
    1.5  | 
    -  | 
    1.6  | 
    -  | 
    1.0  | 
    1.5  | 
    -  | 
  
Others  | 
    -  | 
    -  | 
    -  | 
    -  | 
    W, Co  | 
    -  | 
    -  | 
    -  | 
    W 5.0  | 
    W add  | 
    -  | 
    AI  | 
  
Max. Temperature (ºC)  | 
    1050  | 
    1100  | 
    1100  | 
    1000  | 
    1100  | 
    1150  | 
    1050  | 
    1050  | 
    1200  | 
    1180  | 
    1000  | 
    1100  | 
  
Request the complete technical file of the alloy.
Work other alloys on demand. 
ALLOYS USED IN THE HEATING
ALLOY  |  
    MAXIMUM TEMPERATURE ºC  |  
  |||||||||
AIASI  |  
    WERK STOFF  |  
    Dry air  |  
    Moist air  |  
    N2  |  
    Ar  |  
    EXO  |  
    ENDO  |  
    H2  |  
    75 h2  |  
    Empty  |  
  
NiCr 80  |  
    2.4869  |  
    1200  |  
    1150  |  
    250  |  
    1250  |  
    1100  |  
    1100  |  
    1250  |  
    1250  |  
    1000  |  
  
NiCr 70  |  
    2.4858  |  
    1250  |  
    1150  |  
    1250  |  
    1250  |  
    1200  |  
    1100  |  
    1250  |  
    1250  |  
    1000  |  
  
KA1 et KAPM  |  
    1.4765  |  
    1400  |  
    1200  |  
    1200  |  
    1400  |  
    1150  |  
    1050  |  
    1400  |  
    1200  |  
    1150  |  
  
Request the complete technical file of the alloy.
Work other alloys on demand.